# Raw Mill Stops and Corrosion in the Cement Kiln Gas Path

When the raw mill stops, kiln gas bypasses the mill and goes from the conditioning tower straight to the filter: it loses the mill's cooling and raw material moisture, the tower sprays more water, and more sulfur dioxide reaches the filter and stack. Condensation zones shift with each mode and with every switch.

**Category:** Articles
**Written by:** Edita Rojasova
**Last updated:** Nov 18, 2026
**Source:** https://signals.polylloycoatings.com/articles/raw-mill-stops-kiln-corrosion

---

## Raw Mill Stops and Kiln Gas Corrosion: Key Points

- With an in-line raw mill, kiln gas dries raw material while the mill runs (compound operation) and goes straight from the conditioning tower to the filter when it stops (direct operation).

- When the raw mill stops, the mill no longer takes heat or adds raw material moisture, so the conditioning tower typically carries the whole cooling duty with water spray.

- A running raw mill also captures part of the kiln's sulfur dioxide (SO2) in the raw meal; with the mill stopped, more SO2 reaches the filter and stack.

- Condensation risk moves with the mode: spray-wetted tower walls in direct operation, cooler and wetter mill outlet ducts, filter and stack in compound operation, and dew point crossings at every switch.

- Polylloy's May 2026 International Cement Review (ICR) article puts cement plant acid dew points typically at 120 to 160 °C, so record gas analysis and metal temperatures in both modes.

- Protect steel that still crosses the dew point: FlueGard®-225SQC, an immersion grade, for cement baghouses and ducts to 225 °C; FlueGard-425S for cement conditioning towers and stacks to 425 °C, but not for wetted zones.

When the raw mill stops, kiln gas bypasses the mill and goes from the conditioning tower straight to the filter: it loses the mill's cooling and raw material moisture, the tower sprays more water, and more sulfur dioxide reaches the filter and stack. Condensation zones shift with each mode and with every switch.

## Compound and Direct Operation in the Cement Kiln Gas Path

Compound and direct operation send the same kiln gas along two routes that load the steel differently.

### Two Routes for the Same Kiln Gas

Compound and direct operation are the two modes of a cement kiln with an in-line raw mill. In compound operation the kiln exhaust gas passes through the running raw mill to dry the raw material before the main filter, and in direct operation the raw mill is stopped and the gas goes from the conditioning tower straight to the filter and stack.

The two routes run as follows:

- **Compound operation:** preheater, conditioning tower, raw mill, main filter, fan, stack.

- **Direct operation:** preheater, conditioning tower, main filter, fan, stack.

Layouts vary; the main filter may be an electrostatic precipitator (ESP) rather than a baghouse, and time spent in direct operation is plant-specific.

![Compound and direct kiln gas routes compared, with gas changes, condensation risk zones and bulletin-listed protection]()

### Why Corrosion Follows the Operating Mode

The same steel sees different gas temperature, moisture, sulfur oxides and dust in each mode, so the acid dew point and the coldest metal both move. Assessing one mode misses the exposure of the other.

## What Changes in Kiln Gas When the Raw Mill Stops

Kiln gas changes in temperature, moisture, sulfur oxides and dust when the raw mill stops.

### Gas Temperature

In compound operation the raw mill uses the gas heat to dry raw material, so gas leaves the mill cooler. In direct operation that heat sink is gone, and the conditioning tower must cool the gas to the filter's inlet limit on its own.

### Moisture

Compound operation adds evaporated raw material moisture, partly diluted by mill false air, while direct operation adds the extra tower spray water. Net moisture, and so the acid dew point, differs by mode and by plant, and the ICR article notes that higher moisture raises the acid dew point. Calculate the dew point for each mode separately.

### Sulfur Dioxide and Sulfur Trioxide

Raw meal in a running mill captures part of the kiln SO2, so in direct operation more SO2 passes to the filter and stack. According to the ICR article, a portion of SO2 oxidizes to sulfur trioxide (SO3) with oxygen and catalysts such as iron oxides and alkalis.

SO3 and water vapor form sulfuric acid (H2SO4), raising the acid dew point, typically to 120 to 160 °C in cement plant flue gas, depending on SO3 concentration and moisture.

### Dust Load and Alkaline Buffering

Compound operation carries raw meal dust from the mill to the filter, while direct operation carries kiln dust only. The ICR article notes that alkaline dust on the dirty side can partly neutralize acidic condensate, while the clean side largely lacks that buffer. How much buffering each mode gives is plant-specific.

## Conditioning Tower Spray and Wet Walls in Direct Operation

Conditioning tower spray carries the full cooling duty in direct operation, which makes the tower walls a key zone to watch.

### How Conditioning Towers Get Wet

In direct operation the gas conditioning tower (GCT) sprays more water. Worn nozzles, poor atomization or a setpoint close to the dew point leave droplets that wet the walls or carry into the outlet duct, building damp dust deposits. The ICR article names gas conditioning systems among frequent corrosion zones in cement plants.

### Conditioning Tower Protection

The FlueGard-425S bulletin lists conditioning towers and stacks in cement and lime plants. It is a single-component inorganic polymeric coating rated from ambient to 425 °C (797 °F) with peaks to 500 °C, resistant to SO3, SO2, hydrogen chloride (HCl), carbon dioxide (CO2), nitrogen oxides (NOx) and dust abrasion, with Taber abrasion below 150 mg.

FlueGard-425S is not an immersion grade, so no performance is claimed for it in spray-wetted or condensing wall zones; Polylloy's technical team selects the grade for those zones. Tower limits in a lime context are covered in [lime plant corrosion protection](https://signals.polylloycoatings.com/use-cases/lime-plant-corrosion-protection), and coating behavior under repeated heating and cooling in [hot flue gas duct protection](https://signals.polylloycoatings.com/use-cases/hot-flue-gas-duct-protection).

## Mill Outlet Ducts and the Kiln Baghouse in Compound Operation

Mill outlet ducts and the kiln baghouse take the cooler, wetter gas of compound operation.

### Cooler, Wetter Gas After the Raw Mill

Gas leaving the mill is cooler and carries raw material moisture, so the mill outlet duct, the main filter casing and its clean side run closer to the acid and water dew points. False air at mill seals, rotary feeders and duct joints cools steel locally and, per the ICR article, raises oxygen that can promote SO3 formation.

Corrosion inside a cement plant baghouse is caused by acid condensate wherever metal runs below the dew point, often worst on the clean side and under damp deposits. Both conditions vary with raw mill mode.

### Baghouse and Duct Protection

FlueGard-225SQC is a two-component polymeric alloy listed for baghouses, ESPs and ducts in cement plants, rated to 225 °C (437 °F), resistant to SO3, SO2, HCl, CO2, hydrogen fluoride (HF) and NOx, and immersion-rated. Grade data are on the [FlueGard flue gas coatings](https://www.polylloycoatings.com/fluegard) page.

FlueGard on coal mill baghouses at three cement plants in Mexico was inspected after about 20, 15 and 16 years, with no issues observed, excellent condition and excellent performance reported; only the 2008 unit is specifically FlueGard-225SQC. These are coal mill filters, not kiln main filters. Zone-by-zone outage checks are in the [baghouse corrosion maintenance checklist](https://signals.polylloycoatings.com/articles/baghouse-corrosion-maintenance-checklist).

## Mode Switches, Kiln Stops and Dew Point Crossings

Mode switches and kiln stops add short, sharp exposures on top of steady running.

### Why Each Switch Matters

Each raw mill start or stop changes gas temperature, moisture and SO2 quickly, and spray control can lag, giving wet or cold events at the tower and filter. Cement plant filter casings can corrode early partly for this reason: steel that is dry in one mode can condense acid in the other or during the switch.

Other causes, such as seals, hoppers and the clean side, are covered in the [acid dew point warning signs](https://signals.polylloycoatings.com/listicles/acid-dew-point-corrosion-signs).

### Kiln Stops and Deposits

Polylloy's technical paper on stainless steels and claddings gives the typical sequence: deposition in operation, cooling at shutdown, moisture uptake or condensation, salt dissolution, and localized corrosion beneath retained deposits. Dry operation does not demonstrate that shutdown exposure is benign, and frequent raw mill stops add partial versions of that cycle to the filter and ducts between kiln stops.

## The Steel Stack in Compound and Direct Operation

The steel stack sees both modes at the end of the gas path, where gas is often coolest.

### Stack Exposure by Mode

The ICR article describes stacks as the final, often coldest, stage of the flue gas path, where continued cooling makes crossing the acid dew point more likely. Compound operation tends to send cooler, wetter gas to the stack, while direct operation sends gas with more SO2, so check both modes against the calculated dew point.

FlueGard-425S is listed for stacks in cement and lime, but because it is not an immersion grade, condensing stack sections are a grade decision for Polylloy's technical team. Shell checks are set out in the [steel stack inspection checklist](https://signals.polylloycoatings.com/articles/steel-stack-inspection-checklist).

## How to Manage Corrosion Across Raw Mill on and Off Operation

Managing corrosion across raw mill modes means treating each mode as its own design case.

### Six Steps by Operating Mode

1. Log the operating mode alongside gas analyzer data (SO2, moisture, oxygen) and temperatures, so readings can be split by mode.

2. Calculate the acid dew point for each mode and compare it with minimum metal temperatures at the tower, mill outlet duct, filter, fan and stack.

3. Maintain conditioning tower nozzles and atomization, and set the tower outlet temperature with a margin above the dew point in direct operation, taken from the plant's own standard.

4. Repair insulation and seals on the mill circuit and filter.

5. Inspect each zone at every outage with the mode that stresses it in mind.

6. Protect the steel that still crosses the dew point.

Polylloy's Coating Selection Questionnaire asks for normal temperature range, maximum peaks and their duration and frequency; give these for both modes. Baghouse filters also corrode after emissions upgrades because cooler gas and higher-efficiency filtration leave more steel near the dew point and less alkaline dust on the clean side, as the ICR article explains.

The options are compared in [corrosion protection options after an emissions upgrade](https://signals.polylloycoatings.com/listicles/emissions-upgrade-corrosion-protection).

### Protection in the Kiln Gas Path

FlueGard-225SQC covers the main filter and ducts within 225 °C. FlueGard-425S covers conditioning tower and stack sections within its listing and limit, but it is not claimed for wetted or condensing zones, which Polylloy's technical team assesses per project.

Certified partners apply the coatings, while Polylloy formulates, supplies, specifies, trains and supervises. Surface preparation is SSPC-SP10 (Society for Protective Coatings) / NACE No. 2 near-white with a profile above 3 mils (75 µm), and final heat cured activation is completed during start-up using process heat.

## Deciding Where to Protect First in Your Kiln Gas Path

Deciding where to protect first in the kiln gas path follows three rules:

- Fix spray and seal causes first.

- Protect the zones that cross the dew point in either mode, starting where wall loss is already measured.

- Where metal stays well above the dew point in both modes, a conventional coating may be enough.

To plan it, [book a Coating Performance Review](https://www.polylloycoatings.com/contact) with gas data and metal temperatures for both raw mill modes, equipment type, coated area, location and outage timing.

### FAQs

**What Happens to Kiln Gas When the Raw Mill Stops?**

With the raw mill stopped, kiln gas skips the mill and goes from the conditioning tower straight to the filter and stack. It loses the mill's cooling and raw material moisture, the tower sprays more water to hold the filter inlet temperature, and less sulfur dioxide is captured by raw meal, so more reaches the filter and stack.

**What is the Difference Between Compound and Direct Operation in a Cement Kiln?**

In compound operation the raw mill runs and kiln exhaust gas passes through it to dry the raw material before reaching the main filter. In direct operation the raw mill is stopped and the gas goes from the conditioning tower straight to the filter. Gas temperature, moisture, sulfur dioxide and dust load all differ between the two modes.

**Why Do Cement Plant Filters Fail Early?**

Early corrosion failures in cement plant filters often trace to steel running below the acid dew point at cold spots, on the clean side and under damp hopper dust. Raw mill switching adds to it: steel that stays dry in one mode can condense acid in the other or during the change. Check metal temperatures in both raw mill modes, not one.

**What Causes Corrosion Inside a Cement Plant Baghouse?**

Acid condensate forms wherever baghouse steel runs below the acid dew point of the kiln gas, typically 120 to 160 °C in cement plants according to Polylloy's May 2026 ICR article. The clean side largely lacks alkaline dust buffering and is often more exposed, while damp deposits attack hoppers during shutdowns. Raw mill mode changes shift both effects.

**Why Do Baghouse Filters Corrode After Emissions Upgrades?**

Upgrades often cool the gas and improve filtration, so more steel runs near or below the acid dew point and less alkaline dust reaches the clean side to neutralize condensate. In a kiln with an in-line raw mill, check the new conditions in both compound and direct operation, because the upgrade can change each mode differently.

**Does a Cement Plant Conditioning Tower Need a Coating?**

It needs one where tower steel meets condensate or spray wetting, most often during direct operation when the tower carries the full cooling duty. The FlueGard-425S bulletin lists conditioning towers and stacks in cement and lime plants, rated to 425 °C with peaks to 500 °C, but it is not an immersion grade, so Polylloy's technical team selects the grade for wetted zones.

**Is the Kiln Stack More Corrosive with the Raw Mill on or Off?**

It depends on the plant. Compound operation usually sends cooler, wetter gas to the stack, while direct operation sends gas carrying more sulfur dioxide. Either can take the stack shell below the acid dew point, so calculate the dew point and measure shell temperatures for both modes before deciding where protection is needed.