# How to Calculate Acid Dew Point for Ducts and Stacks: Sulfuric and Hydrochloric

To calculate acid dew point for a flue gas duct, convert the measured water vapor, sulfur trioxide and hydrogen chloride concentrations to partial pressures, then apply a published correlation for sulfuric acid and another for hydrochloric acid. Compare the higher result with the coldest metal temperature in every operating state, and choose protection rated for the hottest.

**Category:** Articles
**Written by:** Edita Rojasova
**Last updated:** Nov 18, 2026
**Source:** https://signals.polylloycoatings.com/articles/acid-dew-point-calculation

---

## Acid Dew Point Calculation: Key Points

- Acid dew point calculation starts from a gas analysis: water vapor, sulfur trioxide (SO3) or sulfuric acid vapor, and hydrogen chloride (HCl), each converted to a partial pressure at the duct's operating pressure.

- Published empirical correlations, used as printed in their original papers, give a sulfuric acid dew point and a separate, usually lower, hydrochloric acid dew point.

- SO3 is the hardest input because routine analyses rarely report it, so measure it or state a sourced estimate.

- Compare the calculated dew point with the coldest metal temperature in every operating state, not with the gas temperature on the control screen.

- Polylloy's May 2026 International Cement Review (ICR) article puts cement plant acid dew points typically at 120 to 160 °C, depending on SO3 and moisture.

- The dew point decides whether steel needs acid protection; the hottest metal temperatures decide the grade, for example StackGard®-255SQW to 255 °C or FlueGard®-225SQC to 225 °C.

To calculate acid dew point for a flue gas duct, convert the measured water vapor, sulfur trioxide and hydrogen chloride concentrations to partial pressures, then apply a published correlation for sulfuric acid and another for hydrochloric acid. Compare the higher result with the coldest metal temperature in every operating state, and choose protection rated for the hottest.

## Acid Dew Point Calculation and What It Tells You

An acid dew point calculation tells you which duct and stack steel will collect acid condensate, and in which operating states.

### Acid Dew Point and Acid Dew Point Corrosion Defined

Acid dew point calculation is the estimate, from a flue gas analysis and published empirical correlations, of the temperature below which sulfuric or hydrochloric acid condenses from the gas onto a surface. The acid dew point is that temperature, and acid dew point corrosion is attack on steel by the condensate wherever metal runs colder than it.

The dew point is a property of the gas, while condensation is a property of the metal surface. Symptoms in service are covered in the [acid dew point warning signs](https://signals.polylloycoatings.com/listicles/acid-dew-point-corrosion-signs) guide.

### Why Calculate Instead of Using a Typical Range

Polylloy's May 2026 ICR article puts the acid dew point typically at 120 to 160 °C in cement plant flue gas, depending on SO3 concentration and moisture. Fuel, raw materials, gas conditioning and operating mode move a plant within or outside that range, and other industries need their own figure. A calculation from the plant's own gas analysis gives a plant number.

## Inputs an Acid Dew Point Calculation Needs

An acid dew point calculation needs four inputs, each taken at the location being assessed: water vapor, SO3 or sulfuric acid vapor, HCl and total gas pressure.

### Water Vapor in the Flue Gas

Moisture by volume comes from the gas analysis in each operating state. It arises from fuel hydrogen, fuel and raw material moisture, gas conditioning and water sprays, as set out in [flue gas composition and the corrosion each component causes](https://signals.polylloycoatings.com/listicles/flue-gas-composition-corrosion). Higher moisture raises the acid dew point, as the ICR article notes.

### Sulfur Trioxide or Sulfuric Acid Vapor

SO3, present as sulfuric acid (H2SO4) vapor once it combines with water, sets the sulfuric acid dew point. According to the ICR article, sulfur enters the cement kiln system mainly as sulfur dioxide (SO2), and a portion oxidizes to SO3 in the presence of oxygen and catalysts such as iron oxides and alkalis.

Routine analyses usually report SO2, not SO3. Either measure SO3 with a recognized sampling method, or estimate it from SO2 with a conversion assumption from a published source for that process, and state which route was used.

False air matters here too. Seal, joint and duct leaks raise oxygen and can promote SO3 formation locally, so a leak can raise the local dew point and cool the steel at the same time.

### Hydrogen Chloride

HCl comes from chlorine in fuels, alternative fuels, waste and raw materials. Take it from the gas analysis or emissions monitoring, and record it separately from SO3, because HCl gets its own dew point calculation.

### Total Pressure, Units and Operating States

Convert each volume fraction to a partial pressure at the duct's actual pressure, in the exact units the chosen correlation uses. Polylloy's Coating Selection Questionnaire asks for gas composition, the normal gas temperature range, maximum peaks, and their duration and frequency. Collect inputs per operating state: full load, low load, start-up, shutdown and mode changes.

## Published Correlations for the Sulfuric Acid Dew Point

Published correlations for the sulfuric acid dew point turn partial pressures into a temperature; two come from Verhoff and Banchero (1974) and from Okkes (1987).

### What the Sulfuric Acid Dew Point Correlations Do

The sulfuric acid dew point correlations are empirical fits to sulfuric acid dew point data. Both the Verhoff and Banchero and the Okkes correlations give the sulfuric acid dew point as a function of the water vapor and sulfuric acid (or SO3) partial pressures.

Compute the partial pressures, insert them in the units each paper states, solve for temperature, then convert the result. Copy each equation, its constants, temperature scale and validity range from the original paper, not from a secondary website.

### Choosing and Checking a Sulfuric Acid Correlation

Different correlations give different answers for the same gas, so run both and report both; the spread is a reason for margin. Outside a correlation's published validity range, label the result an extrapolation.

A correlation predicts where condensation begins at equilibrium in the bulk gas. It does not predict a corrosion rate or conditions under a deposit, so a worked example is only as good as the plant data behind it.

## Calculating the Hydrochloric Acid and Water Dew Points

The hydrochloric acid and water dew points complete the calculation, because a sulfuric acid result alone misses condensation on colder metal.

### Hydrochloric Acid Dew Point

The hydrochloric acid dew point is calculated with its own published correlation from the water vapor and HCl partial pressures. It is usually lower than the sulfuric acid dew point, so HCl condensate tends to appear on colder steel: corners, doors, uninsulated stiffeners and equipment cooling at shutdown.

Chlorine-rich gas from alternative fuels or waste makes this matter. On stainless steel, chloride condensate drives pitting, as explained in [why 316 stainless corrodes in flue gas](https://signals.polylloycoatings.com/articles/316-stainless-flue-gas-corrosion).

### Water Dew Point

The water dew point follows from the water vapor partial pressure using standard steam tables; below it, liquid water forms and dissolves SO2 and HCl. A shutdown or start-up can take cooling steel through all three dew points.

## Comparing the Acid Dew Point with Metal Temperature, Not Gas Temperature

Comparing the acid dew point with metal temperature, rather than gas temperature, turns the number into a corrosion map.

### The Coldest Metal Decides Where Acid Condenses

Acid dew point corrosion starts where the metal surface, not the bulk gas, falls below the calculated dew point. The ICR article notes that as gases cool towards the acid dew point, sulfuric and hydrochloric acid vapors condense, and even a thin acidic film can significantly accelerate corrosion.

Cold metal sits at stiffeners, flanges, doors, supports, uninsulated corners and false air points, and the fixes are covered in the [flue gas ductwork design rules](https://signals.polylloycoatings.com/listicles/flue-gas-ductwork-design-rules). Stacks often run at the lowest temperatures in the system, and gas keeps cooling as it rises.

### Measuring Metal Temperature in Each Operating State

Use infrared thermography on the casing and contact thermocouples at known cold points, in every operating state. The Coating Selection Questionnaire also asks about external insulation and heat sinks such as fins and flanges, since both affect local metal temperature.

### Why a Few Degrees Below the Dew Point is Not Safe

Condensate strength and corrosion rate both change with how far below the dew point the metal runs, so a dew point says where acid forms, not how fast steel is lost. Treat any metal at or below the calculated dew point as condensing service.

## Applying a Margin and Choosing a Coating Service Limit

Applying a margin means checking both ends: the coldest metal against the dew point and the hottest metal against a coating service limit.

### The Lower Margin: Coldest Metal Against the Dew Point

If the coldest metal stays above the higher calculated dew point plus a design margin in every state, acid condensation in normal running is unlikely. Take the margin from a published design guide or the owner's standard; Polylloy publishes no margin figure. Shutdowns still cross the dew point.

Where metal stays well above the dew point and the gas carries little acid-forming content, a conventional coating may be enough; see the [signs a conventional coating is enough](https://signals.polylloycoatings.com/listicles/conventional-coating-enough-signs).

### The Upper Margin: What Temperature a Stack Coating Needs to Survive

A stack or duct coating has to survive the hottest continuous metal temperature and the excursions above it, not the dew point. Choose a grade whose continuous limit covers the continuous metal temperature, and confirm excursion peak, duration and frequency with Polylloy's technical team, because bulletins state limits, not durations. Three Polylloy grades are bulletin-listed for ducts and stacks:

- **StackGard-255SQW:** to 255 °C (491 °F), for chimneys of industrial plants; details on the [StackGard chimney coating](https://www.polylloycoatings.com/stackgard) page.

- **FlueGard-225SQC:** to 225 °C (437 °F), for baghouses, electrostatic precipitators (ESPs) and ducts in cement plants and waste incinerators, and chimneys in power plants and refineries.

- **FlueGard-425S:** to 425 °C (797 °F) with peaks to 500 °C, for conditioning towers and stacks in cement and lime, and ducts and chimneys in power plants and refineries.

Spike values and the full comparison are on [Polylloy coating grades by temperature and gas chemistry](https://signals.polylloycoatings.com/listicles/coating-grades-temperature-chemistry). FlueGard-225SQC is immersion-rated; StackGard-255SQW and FlueGard-425S are not.

### Reading Both Margins Together

Read the margins in order: calculated dew points, coldest metal by state, hottest metal by state and the excursion profile, then the cold and hot checks. Gas chemistry still filters the shortlist: the FlueGard-225SQC bulletin lists resistance to SO3, SO2, HCl, carbon dioxide (CO2), hydrogen fluoride (HF) and nitrogen oxides (NOx), while the StackGard-255SQW bulletin lists SO3, SO2, HCl and NOx.

![Acid dew point decision path: gas inputs, sulfuric, hydrochloric and water dew points, coldest metal check, three outcomes]()

Grade data are on the [FlueGard flue gas coatings](https://www.polylloycoatings.com/fluegard) page.

## Limits of an Acid Dew Point Calculation

An acid dew point calculation describes the bulk gas, and that sets its limits.

### What an Acid Dew Point Calculation Cannot See

Polylloy's technical paper on stainless steels and claddings notes that bulk flue-gas chemistry may not describe the environment at the metal surface, and that deposits can retain moisture and concentrate soluble salts. When SO3 is estimated rather than measured, that uncertainty dominates the result. A direct acid dew point probe can cross-check a close call.

## Deciding What Your Acid Dew Point Result Means for Ducts and Stacks

Deciding what an acid dew point result means comes down to three outcomes:

- Metal stays above the dew point with margin in every state: conventional protection may be enough.

- Metal crosses the dew point in some states: fix insulation and seals, then protect the steel that still crosses.

- Metal runs below the dew point in normal service: protect the steel and review gas temperature setpoints.

Certified partners apply Polylloy coatings; Polylloy formulates, supplies, specifies, trains and supervises. Surface preparation is SSPC-SP10 (Society for Protective Coatings) / NACE No. 2 near-white with a profile above 3 mils (75 µm), and for heat-cured grades, final heat cured activation is completed during start-up using process heat.

To test your result against a grade, [book a Coating Performance Review](https://www.polylloycoatings.com/contact) with a recent gas analysis, metal temperatures by operating state, equipment type, coated area, location and outage timing.

### FAQs

**How Do You Calculate the Acid Dew Point of Flue Gas?**

Take a gas analysis with water vapor, sulfur trioxide and hydrogen chloride, convert each concentration to a partial pressure at the duct's pressure, then apply a published sulfuric acid dew point correlation and a separate hydrochloric acid correlation, in the units each paper specifies. Repeat for every operating state and compare the results with measured metal temperatures.

**What is Acid Dew Point Corrosion?**

Acid dew point corrosion is attack on steel by sulfuric or hydrochloric acid that condenses from flue gas wherever the metal is colder than the gas's acid dew point. Polylloy's May 2026 International Cement Review article puts that dew point typically at 120 to 160 °C in cement plant flue gas, depending on sulfur trioxide and moisture.

**What Temperature Does a Stack Coating Need to Survive?**

A stack coating has to survive the hottest continuous metal temperature and the excursions above it, not the acid dew point. The dew point shows that acid protection is needed; the hot end picks the grade. StackGard-255SQW, for example, is rated to 255 °C for industrial chimneys, and Polylloy's technical team confirms excursion duration and frequency per project.

**Is the Hydrochloric Acid Dew Point Higher or Lower Than the Sulfuric Acid Dew Point?**

Usually lower. Hydrogen chloride needs colder metal to condense than sulfuric acid vapor does, so hydrochloric acid tends to appear at the coldest spots and during cool-down. Calculate it separately with its own published correlation, because chlorine-rich gas from alternative fuels or waste can make hydrochloric acid the condensate that matters at doors, corners and stiffeners.

**How Do You Estimate Acid Dew Point Without an SO3 Measurement?**

Estimate sulfur trioxide from the measured sulfur dioxide with a conversion assumption taken from a published source for your process, and state it as an assumption. Because sulfur trioxide drives the sulfuric acid dew point, that estimate dominates the uncertainty. Where the decision is close, measure sulfur trioxide or cross-check with a direct dew point probe.

**How Does Acid Dew Point Corrosion Start in Flue Gas Equipment?**

It starts where a metal surface falls below the acid dew point of the gas: a stiffener, door frame, uninsulated corner, false air leak or stack section that runs colder than the bulk gas. Acid condenses there as a thin film, and even a thin acidic film can significantly accelerate corrosion, according to Polylloy's May 2026 ICR article.

**Does Keeping Flue Gas Above the Acid Dew Point Prevent Corrosion?**

Not on its own. The gas can sit above the dew point while cold metal at leaks, flanges or uninsulated zones sits below it, shutdowns can take the steel through the dew point, and deposits can hold moisture and acid against the steel. Keep metal above the dew point where possible and protect the steel that cannot be kept there.